The pH value determination of pyrolysis products is a standardized fire-safety test that quantifies the acidity or alkalinity of the aqueous solution formed when gases evolved from a thermally decomposed material are absorbed in water. Commonly performed on cable insulation and sheathing materials in accordance with IEC 60754-2, EN 50267-2-2, and GB/T 17650.2, the test is a key indicator of the corrosion potential and toxic gas hazard of combustion products. This article explains the technical principle, sample requirements, test procedure, acceptance criteria, and typical applications of the pyrolysis product pH determination experiment.
Technical Overview
The pH value determination of pyrolysis products evaluates the degree of acidity (corrosivity) of the gases released when a polymeric material is decomposed under controlled heating conditions. During a fire, halogen-containing polymers such as PVC can release significant quantities of hydrogen chloride or hydrogen bromide. These acidic gases are highly corrosive to electronic equipment, metal structures, and concrete, and they pose a serious hazard to human respiratory systems when inhaled.
In the test, a weighed sample is pyrolyzed in a tube furnace, and the evolved gases are bubbled through an absorption vessel containing high-purity water. The pH value of the resulting solution is then measured with a calibrated pH meter. A low pH indicates a high concentration of acidic decomposition products, while a pH close to neutral indicates that the material releases little or no corrosive acid gas when burned.
The most widely applied methodology is defined in the following standards and their equivalents:
- IEC 60754-2 – Test on gases evolved during combustion of materials from cables, Part 2: Determination of degree of acidity (corrosivity) of gases by pH and conductivity measurements
- EN 50267-2-2 / BS EN 50267-2-2 – European adoption of the same method
- GB/T 17650.2 – Chinese national standard corresponding to IEC 60754-2
For low-smoke halogen-free (LSZH, LSOH, LSHF) materials, the typical acceptance requirement is a pH value of not less than 4.3, usually assessed together with a conductivity limit of not more than 10 μS/mm.
Testing Samples
Cable and Wire Materials
The most common test objects are polymeric compounds taken from finished cables and wires, including insulation, sheathing, outer jackets, and bedding layers. Samples are typically cut or peeled directly from the cable product so that the test reflects the actual material delivered to the market.
Polymeric Raw Materials and Compounds
Compound manufacturers submit raw pellets or granules for evaluation during formulation development, incoming quality control, and batch release. Typical materials include cross-linked polyethylene (XLPE), polyethylene (PE), ethylene-vinyl acetate (EVA) or polyolefin-based halogen-free flame-retardant compounds, thermoplastic elastomers (TPE), and PVC compounds for comparison purposes.
Other Polymer-Based Products
The method can also be applied to other combustible polymeric components where combustion-gas corrosivity is a concern, such as connector housings, cable accessories, gaskets, foamed sealing materials, and interior decoration materials used in enclosed spaces.
Testing Items
The core testing item is the pH value of the aqueous solution that has absorbed the pyrolysis gases. In practice, the test is normally executed together with its companion parameter, and the full scope includes:
- pH value of the absorption solution after pyrolysis of the sample
- Conductivity of the same solution (measured simultaneously under IEC 60754-2)
- Verification of apparatus and reagent blanks to ensure the water and system contribute no measurable acidity
Testing Methods
Apparatus
The standard test configuration consists of an electric tube furnace capable of maintaining the pyrolysis temperature, a quartz or ceramic combustion tube, a combustion boat for the sample, gas washing bottles in series containing deionized water, a controlled air supply with a flow meter, and a calibrated pH meter equipped with a combined glass electrode. A conductivity measuring cell and a temperature-controlled bath are used when the companion conductivity measurement is performed.
Sample Preparation
A test portion of approximately 1 g is taken from the material and cut into small pieces of a few millimeters to ensure uniform and reproducible pyrolysis. Samples are identified, weighed accurately, and placed in a clean combustion boat. When finished cables are tested, the insulation or sheath is separated from conductors and other layers before cutting.
Test Procedure
The general procedure, following the sequence specified in IEC 60754-2 and its equivalent standards, is as follows:
- Charge the wash bottles with a defined volume of high-purity deionized water and connect them in series downstream of the combustion tube.
- Establish a controlled stream of air through the system at the flow rate specified in the standard.
- Bring the furnace to the specified pyrolysis temperature, commonly around 800 °C, and stabilize it.
- Insert the combustion boat containing the weighed sample into the hot zone of the tube and maintain pyrolysis for the prescribed dwell time.
- After pyrolysis is complete, rinse the downstream tubing and connections into the absorption water and bring the solution to its defined final volume.
- Measure the pH of the solution with a calibrated pH meter at a controlled temperature, commonly 23 °C ± 2 °C, and record the result.
- Where required, measure the conductivity of the same solution for the combined acidity assessment.
Acceptance Criteria
Under IEC 60754-2 and EN 50267-2-2, a material is considered to release no significant amount of corrosive acid gas when the absorption solution has a pH of not less than 4.3 and a conductivity of not more than 10 μS/mm. Materials failing the pH limit, such as conventional PVC compounds that liberate hydrogen chloride, are classified as acidic and are excluded from halogen-free, low-corrosivity applications.
Applications
Pyrolysis product pH determination is a routine requirement in the cable industry and in broader fire-safety engineering. Typical applications include:
- Qualification and type testing of low-smoke zero-halogen (LSZH/LSHF) cables for buildings, data centers, tunnels, and mass-transit systems
- Compliance demonstration for cable product standards and purchaser specifications that call up IEC 60754-2 or EN 50267-2-2
- Research and development of halogen-free flame-retardant compounds, where pH results guide the selection of polymers, mineral fillers, and additives
- Incoming inspection and batch quality control of insulation and sheathing compounds at cable factories
- Verification of materials used in railway, shipboard, offshore, and other enclosed-environment installations where corrosive combustion gases cause disproportionate damage
- Comparative fire-hazard studies of polymeric materials in academic and industrial laboratories
FAQ
What does a low pH result indicate?
A low pH indicates that the material released acidic gases, most commonly hydrogen chloride or hydrogen bromide from halogenated polymers, during thermal decomposition. These gases are corrosive to equipment and structures and are toxic to occupants during a fire.
What are the pass criteria for halogen-free materials?
According to IEC 60754-2 and EN 50267-2-2, the absorption solution should have a pH of at least 4.3 and a conductivity not exceeding 10 μS/mm. Both criteria are assessed on the same solution after the pyrolysis run.
How much sample is required for the test?
A test portion of approximately 1 g is typically specified. The material is cut into small pieces to ensure consistent pyrolysis, and the exact mass is recorded for traceability of the test.
Why is pH usually measured together with conductivity?
The two parameters complement each other. pH reflects the acid strength of dissolved gases, while conductivity reflects the total concentration of ionized species. Some species contribute measurably to conductivity without strongly shifting pH, so the combined assessment gives a more complete picture of combustion-gas corrosivity.
How does this test differ from IEC 60754-1?
IEC 60754-1 determines the halogen acid gas content of evolved gases by quantitative chemical analysis, whereas IEC 60754-2 assesses the overall degree of acidity of the gas absorption solution through pH and conductivity. Both are commonly required for a complete corrosion-hazard evaluation of cable materials.
Can the test be performed by any laboratory?
The method requires a tube furnace, gas absorption train, and calibrated pH and conductivity instrumentation. It is routinely carried out by accredited third-party laboratories as well as manufacturer laboratories operating under recognized quality management systems, ensuring results are comparable and accepted across supply chains.
Why Choose ZKGX?
- State-of-the-art analytical equipment
- Highly qualified scientific team
- Fast turnaround time
- Competitive pricing