Global Global Algérie Français Algeria English Angola Português Angola English Argentina Español Argentina English Australia English Austria Deutsch Austria English Azerbaijan English Azerbaijan Русский Bahrain English Bangladesh English Belgium English Belgium Français Belgium Nederlands Brazil Português Brazil English Bulgaria български Bulgaria English Cameroon English Cameroon Français Canada English Canada Français Chile Español Chile English China 中文 China 日本語 China English Colombia Español Colombia English Croatia English Czech Republic Čeština Czech Republic English Denmark English Djibouti English Ecuador Español Ecuador English Egypt English Estonia English Ethiopia English Finland Suomi Finland English France Français France English Georgia English Georgia Русский Germany Deutsch Germany English Ghana English Greece Ελληνικά Greece English Guatemala Español Guatemala English Hong Kong, China English Hong Kong, China 中文 Hungary Magyar Hungary English India English Indonesia English Iraq English Ireland English Italy Italiano Italy English Ivory Coast Français Ivory Coast English Japan 日本語 Japan English Jordan English Kazakhstan Русский Kazakhstan English Kenya English Kuwait English Kyrgyzstan Русский Kyrgyzstan English Latvia English Lithuania English Malaysia English Mauritius English Mauritius français (Maurice) Mexico Español Mexico English Moldova Română Moldova English Mongolia English Morocco English Morocco Français Mozambique Português Mozambique English Netherlands Nederlands Netherlands English New Zealand English Nigeria English Norway English Oman English Pakistan English Paraguay Español Paraguay English Peru Español Peru English Philippines English Poland Polski Poland English Portugal Português Portugal English Qatar English Republic of Korea 한국어 Republic of Korea English Romania Română Romania English Saudi Arabia English Serbia Српски Serbia English Singapore English Slovakia English Slovenia English South Africa English Spain English Spain Español Sri Lanka English Sweden English Switzerland Deutsch Switzerland Français Switzerland Italiano Switzerland English Tanzania English Thailand ไทย Thailand English Togo English Togo Français Tunisia English Tunisia Français Türkiye Türkçe Türkiye English Turkmenistan Русский Turkmenistan English Ukraine Українська Ukraine English United Arab Emirates English United Kingdom English Uruguay Español Uruguay English USA English Uzbekistan English Uzbekistan Русский Vietnam Tiếng Việt Vietnam English

Boiling Method Water Absorption Test: Standards, Procedure, and Applications

The boiling method water absorption test is a standardized gravimetric technique used to determine the open porosity and water absorption of ceramic tiles, fired whiteware, and related sintered materials. Conforming to internationally recognized standards such as ISO 10545-3, GB/T 3810.3, and ASTM C373, this test provides critical data for product classification, quality control, and durability assessment. This article explains the testing principle, specimen requirements, detailed procedure, calculation methods, and typical applications of the boiling method water absorption test.

Technical Overview

Water absorption is one of the most important physical properties for evaluating the degree of vitrification, pore structure, and long-term durability of fired ceramic materials. The boiling method water absorption test measures the percentage by mass of water that a dried specimen absorbs after being boiled in water for a defined period and then cooled while fully immersed. During boiling, the expansion of heated air and the formation of water vapor within the open pores expel trapped gases, allowing water to penetrate and saturate the pore network.

The test is primarily governed by ISO 10545-3 and its Chinese equivalent GB/T 3810.3, which cover the determination of water absorption, apparent porosity, apparent relative density, and bulk density of ceramic tiles. ASTM C373 describes related procedures for fired ceramic whiteware products and ceramic tiles. Test results are used to classify products according to ISO 13006, GB/T 4100, and EN 14411, which define absorption-based groups such as porcelain (BIa), vitrified (BIb), and semi-vitrified tiles (BIIa, BIIb, BIII).

  • Property measured: water absorption, expressed as mass percentage of the dry specimen
  • Core standards: ISO 10545-3, GB/T 3810.3, EN ISO 10545-3, ASTM C373
  • Specimen quantity: typically 10 tiles or representative specimens per lot
  • Key outputs: water absorption (E), and optionally apparent porosity, bulk density, and apparent relative density

Testing Samples

Ceramic Tiles

Dry-pressed and extruded ceramic tiles, including porcelain tiles, glazed and unglazed wall and floor tiles, polished tiles, and rustic tiles, are the most common test subjects. Whole tiles are preferred whenever practical, as the standards generally require testing complete units to capture the true pore structure of the finished product.

Extruded Ceramic Products

Split tiles, roofing tiles, terracotta façade panels, and clay pipes produced by extrusion are routinely evaluated using the boiling method. These products often exhibit higher and more variable absorption values, making saturation-based testing essential for batch conformity assessment.

Fired Whiteware and Porous Technical Ceramics

Sanitaryware fragments, tableware, electrical porcelain, porous refractory products, and other sintered ceramic components can also be tested. For large or irregular items, representative cut specimens with clean, unsealed fracture or cut surfaces are prepared in accordance with the applicable standard.

Testing Items

The boiling method supports several interrelated determinations. Depending on whether hydrostatic weighing is performed, the following results can be reported:

  • Water absorption (E): the ratio of the mass of absorbed water to the dry mass of the specimen, expressed as a percentage
  • Apparent porosity (P): the volume of open pores expressed as a percentage of the exterior volume of the specimen, derived using the suspended mass
  • Bulk density (B): the dry mass per unit exterior volume, typically expressed in g/cm³
  • Apparent relative density (R): the ratio of the dry mass to the volume of solid material excluding open pores

For most routine quality control and certification purposes, water absorption is the primary reported item, while the derived properties are included when a complete material characterization is required.

Testing Methods

Principle

A specimen is first oven-dried to constant mass and weighed to obtain the dry mass (m1). It is then boiled in water for a specified duration, cooled while immersed, surface-dried, and weighed again to obtain the saturated mass (m2). The mass difference relative to the dry mass represents the water absorbed by the open pores.

Apparatus

  • Forced-convection drying oven capable of maintaining 110 °C ± 5 °C
  • Balances with an accuracy of at least 0.01 % of the mass being weighed
  • Heat-resistant boiling vessel and heating source, with a provision for maintaining water level
  • Desiccator with silica gel for cooling dried specimens without moisture pickup
  • Damp chamois leather or lint-free cloth for surface drying
  • Hydrostatic weighing assembly with wire basket and immersion tank (for porosity and density determination)
  • Clean water, preferably demineralized or of drinking quality

Procedure

  • Dry the specimens at 110 °C ± 5 °C until constant mass, verified when the difference between two successive weighings at 24-hour intervals does not exceed 0.1 %
  • Cool the specimens in a desiccator to room temperature and weigh each one to record the dry mass m1
  • Place the specimens in the boiling vessel, separated from each other and from the vessel walls, and cover them with water to a depth of at least 50 mm
  • Boil the water and maintain gentle boiling for 2 hours, ensuring the specimens remain fully submerged; replenish evaporated water as necessary
  • Cool the water to room temperature, adding cold water if required, and leave the specimens immersed for a further 4 hours ± 15 minutes
  • Remove each specimen individually, remove surface water with a wrung, damp chamois leather, and immediately weigh to record the saturated mass m2
  • Where required, determine the suspended mass m3 by hydrostatic weighing immediately after the saturated weighing

Calculation and Expression of Results

Water absorption is calculated as E = (m2 - m1) / m1 × 100, expressed as a percentage. When hydrostatic data are collected, apparent porosity is calculated as P = (m2 - m1) / (m2 - m3) × 100, bulk density as B = m1 / (m2 - m3), and apparent relative density as R = m1 / (m1 - m3), with the density of water taken as 1 g/cm³. Results are generally reported to one decimal place, showing individual values and the mean for the full set of specimens.

Classification Criteria

Based on ISO 13006 and GB/T 4100 for dry-pressed tiles, the mean water absorption determines the product group:

  • Group BIa (impervious, porcelain): E ≤ 0.5 %
  • Group BIb (vitrified): 0.5 % < E ≤ 3 %
  • Group BIIa: 3 % < E ≤ 6 %
  • Group BIIb: 6 % < E ≤ 10 %
  • Group BIII (non-vitrified): E > 10 %

Applications

The boiling method water absorption test is widely applied across the ceramics industry and construction sector:

  • Factory quality control of tile production, monitoring pressing moisture, firing temperature, and kiln uniformity
  • Product classification and conformity marking against ISO 13006, GB/T 4100, and EN 14411 requirements
  • Durability assessment, since low water absorption correlates strongly with resistance to freeze-thaw damage and outdoor weathering
  • Verification of adhesive compatibility, as absorption behavior influences bond strength with cementitious adhesives
  • Research and development of body formulations, glaze fit studies, and sintering optimization programs
  • Independent verification by accredited third-party laboratories for import and export compliance, tender submissions, and dispute resolution

FAQ

What is the boiling method water absorption test?

It is a gravimetric test in which an oven-dried specimen is boiled in water for 2 hours, cooled while immersed for 4 hours, surface-dried, and reweighed. The percentage mass gain relative to the dry mass is reported as the water absorption, reflecting the volume of open interconnected pores in the fired body.

Which standards specify this test?

The boiling method is specified in ISO 10545-3, GB/T 3810.3, and EN ISO 10545-3 for ceramic tiles, and in ASTM C373 for fired ceramic whiteware products. Classification limits are defined in ISO 13006, GB/T 4100, and EN 14411.

How does the boiling method differ from the vacuum method?

The boiling method saturates pores by thermally expelling trapped air, while the vacuum method evacuates air under reduced pressure before water introduction. The vacuum method achieves more complete saturation and is often preferred for very low absorption products such as porcelain tiles; the boiling method remains the classical, widely accepted approach for routine classification and quality control.

Why is controlling the drying and wiping steps important?

Incomplete drying understates the dry mass, while over-wiping after saturation draws water out of the pores. Both errors distort the result, so constant-mass drying, desiccator cooling, and consistent surface drying with a damp chamois leather are essential for reproducibility.

How should specimens be selected and how many are needed?

Specimens should be representative of the production lot, free from visible cracks and glaze defects that could bias results. The standards typically require 10 tiles or specimens per test, and individual values together with the mean should be reported.

What does a high water absorption value indicate?

Elevated absorption usually indicates underfiring, insufficient vitrification, or a highly porous body structure. Such products are more susceptible to frost damage, staining, and strength loss in wet service conditions, and they fall into less demanding application categories under the classification standards.

Why Choose ZKGX?

  • State-of-the-art analytical equipment
  • Highly qualified scientific team
  • Fast turnaround time
  • Competitive pricing