Global Global Algérie Français Algeria English Angola Português Angola English Argentina Español Argentina English Australia English Austria Deutsch Austria English Azerbaijan English Azerbaijan Русский Bahrain English Bangladesh English Belgium English Belgium Français Belgium Nederlands Brazil Português Brazil English Bulgaria български Bulgaria English Cameroon English Cameroon Français Canada English Canada Français Chile Español Chile English China 中文 China 日本語 China English Colombia Español Colombia English Croatia English Czech Republic Čeština Czech Republic English Denmark English Djibouti English Ecuador Español Ecuador English Egypt English Estonia English Ethiopia English Finland Suomi Finland English France Français France English Georgia English Georgia Русский Germany Deutsch Germany English Ghana English Greece Ελληνικά Greece English Guatemala Español Guatemala English Hong Kong, China English Hong Kong, China 中文 Hungary Magyar Hungary English India English Indonesia English Iraq English Ireland English Italy Italiano Italy English Ivory Coast Français Ivory Coast English Japan 日本語 Japan English Jordan English Kazakhstan Русский Kazakhstan English Kenya English Kuwait English Kyrgyzstan Русский Kyrgyzstan English Latvia English Lithuania English Malaysia English Mauritius English Mauritius français (Maurice) Mexico Español Mexico English Moldova Română Moldova English Mongolia English Morocco English Morocco Français Mozambique Português Mozambique English Netherlands Nederlands Netherlands English New Zealand English Nigeria English Norway English Oman English Pakistan English Paraguay Español Paraguay English Peru Español Peru English Philippines English Poland Polski Poland English Portugal Português Portugal English Qatar English Republic of Korea 한국어 Republic of Korea English Romania Română Romania English Saudi Arabia English Serbia Српски Serbia English Singapore English Slovakia English Slovenia English South Africa English Spain English Spain Español Sri Lanka English Sweden English Switzerland Deutsch Switzerland Français Switzerland Italiano Switzerland English Tanzania English Thailand ไทย Thailand English Togo English Togo Français Tunisia English Tunisia Français Türkiye Türkçe Türkiye English Turkmenistan Русский Turkmenistan English Ukraine Українська Ukraine English United Arab Emirates English United Kingdom English Uruguay Español Uruguay English USA English Uzbekistan English Uzbekistan Русский Vietnam Tiếng Việt Vietnam English

ASTM G48 Pitting Corrosion Testing: Methods, Samples, Procedures, and Applications

ASTM G48 is the internationally recognized standard for evaluating the pitting and crevice corrosion resistance of stainless steels and related alloys in ferric chloride solution. This accelerated laboratory test provides critical data such as mass loss, pit density and depth, and the critical pitting temperature (CPT), enabling engineers to rank, qualify, and accept materials for aggressive chloride-bearing environments. This article explains the scope of ASTM G48, its test methods, sample requirements, evaluation procedures, and typical industrial applications.

Technical Overview

ASTM G48, Standard Test Methods for Pitting and Crevice Corrosion Resistance of Stainless Steels and Related Alloys by Use of Ferric Chloride Solution, is one of the most widely used accelerated corrosion tests for austenitic, duplex, super austenitic, and nickel-base corrosion-resistant alloys. The test exposes polished metal coupons to an acidic, highly oxidizing ferric chloride solution, which drives localized breakdown of the passive film and promotes pitting and crevice attack. The results are not intended to predict service life in any specific environment; instead, they provide a reproducible basis for alloy ranking, quality control, weld procedure qualification, and material acceptance.

The standard comprises six test methods, each addressing a different aspect of localized corrosion:

  • Method A – Ferric chloride pitting test at fixed temperature (typically 22 °C or 50 °C) with mass-loss and pit evaluation.
  • Method B – Ferric chloride crevice test using coupons fitted with crevice-forming assemblies.
  • Method C – Critical pitting temperature (CPT) determination for stainless steels.
  • Method D – Critical crevice temperature (CCT) determination for stainless steels.
  • Method E – Critical pitting temperature determination for nickel-base and chromium-bearing alloys.
  • Method F – Critical crevice temperature determination for nickel-base and chromium-bearing alloys.

CPT and CCT values obtained from Methods C through F generally correlate with the pitting resistance equivalent number (PREN), commonly calculated as %Cr + 3.3 × %Mo + 16 × %N (with tungsten counted as 0.5 × %W added to molybdenum in some conventions). Related standards frequently used alongside ASTM G48 include ASTM G1 (cleaning and evaluating corrosion specimens), ASTM G31 (laboratory immersion corrosion testing), ASTM G78 (crevice corrosion testing in seawater), and ASTM A923 (detection of detrimental intermetallic phases in duplex stainless steels, whose Method C uses a similar ferric chloride exposure).

Testing Samples

Plate, Sheet, and Strip Coupons

Flat rectangular coupons (commonly on the order of 50 mm × 25 mm) are sheared or machined from mill products. Edges are deburred and ground to remove deformed or heat-affected metal from cutting, and the exposed faces are prepared to a consistent, documented surface finish (typically wet-ground to a defined grit) so that results from different materials are comparable.

Welded Specimens

Cross-weld coupons containing base metal, heat-affected zone (HAZ), and weld metal are tested to verify that the welding process has not degraded localized corrosion resistance. Preferential attack on the weld metal or HAZ indicates precipitation of detrimental phases, oxidation, or loss of alloying elements such as nitrogen. Welded super duplex and duplex grades are frequently screened with a fixed-temperature ferric chloride exposure combined with metallographic examination.

Pipe and Tube Samples

Coupons are cut from pipe or tube walls, either flattened or tested in their as-formed curvature depending on the specification. Both internal (ID) and external (OD) surfaces can be evaluated, which is important for tubing intended for seawater cooling, umbilicals, and downhole service.

Forgings, Castings, Bars, and Finished Components

Representative coupons may be machined from forgings, castings, bar stock, or actual fabricated components such as valve bodies, flanges, pump impellers, and fasteners. Because cast and forged structures differ from wrought plate, sampling location and orientation are agreed with the purchaser before testing.

Specimen Preparation

All specimens are identified by marking, degreased with a suitable solvent, rinsed, dried, and weighed to the nearest 0.001 g or better. Dimensions are measured accurately so that the exposed surface area can be calculated and corrosion rates normalized. Each specimen is tested individually in fresh solution to prevent cross-contamination between dissimilar alloys.

Testing Items

Depending on the specified method and acceptance criteria, an ASTM G48 test program can report the following results:

  • Presence or absence of pitting corrosion and crevice corrosion after exposure.
  • Mass loss and calculated corrosion rate (for example, in mdd or mm/year).
  • Pit density (number of pits per unit area) and pit size distribution.
  • Average and maximum pit depth, determined by optical microscopy or cross-sectioning.
  • Location of attack (base metal, weld metal, HAZ, cut edges, or under crevice formers).
  • Critical pitting temperature (CPT) for Methods C and E.
  • Critical crevice temperature (CCT) for Methods D and F.
  • Photographic documentation of specimen surfaces before and after testing.

Testing Methods

Test Solution and Apparatus

The standard test solution contains approximately 6 % ferric chloride (FeCl₃), prepared by dissolving 100 g of ferric chloride hexahydrate (FeCl₃·6H₂O) in 900 mL of distilled or deionized water. The resulting solution is strongly acidic and highly oxidizing, making it far more aggressive toward passive alloys than natural seawater. Specimens are supported on glass cradles or hooks in glass vessels, fully immersed in a controlled volume of fresh solution (typically at least 100 mL per specimen), and maintained at temperature in a water or oil bath with tight control, especially for stepped-temperature CPT and CCT determinations.

Method A – Ferric Chloride Pitting Test

Coupons are immersed for 72 hours at 22 ± 2 °C, or at 50 ± 2 °C when testing more resistant alloys or when a specification demands greater severity. After exposure, the specimens are cleaned in accordance with ASTM G1, reweighed, and examined at magnifications up to about 20×. The report includes mass loss, calculated corrosion rate, and a description of pitting (number, size, and location of pits). Acceptance is commonly defined by the purchaser, for example "no pitting at 20× magnification" or a maximum allowable corrosion rate.

Method B – Ferric Chloride Crevice Test

Specimens are fitted with crevice-forming assemblies, classically a cylindrical coupon contacted by two polymer blocks secured with elastomer bands, creating defined crevice sites. After the exposure period, the assemblies are disassembled and the crevice surfaces are inspected for attack. The extent and depth of crevice corrosion, together with mass loss, are reported.

Method C – Critical Pitting Temperature (Stainless Steels)

The CPT is the lowest solution temperature at which pitting initiation is observed. Testing begins at a temperature below the expected CPT, and specimens are exposed in fresh solution for 24 hours at each step. If no pitting is detected, the temperature is raised in increments (commonly 10 °C, with finer steps near the transition for improved resolution) until attack occurs. CPT is a powerful ranking parameter; typical literature values range from below 10 °C for standard austenitic grades such as 316L, around 20 °C for duplex 2205, approximately 40 °C or higher for super duplex and 6 Mo super austenitic alloys, and above the practical limits of the solution for many nickel-base alloys.

Method D – Critical Crevice Temperature (Stainless Steels)

Method D follows the same stepped-temperature logic as Method C but uses coupons fitted with crevice assemblies. The CCT is the lowest temperature at which crevice corrosion is detected. Because crevice corrosion initiates more readily than pitting, CCT values are always lower than CPT values for the same alloy, and the CPT–CCT gap is an important design consideration for flanged joints and gasketed surfaces.

Methods E and F – CPT and CCT for Nickel-Base Alloys

Methods E and F extend the stepped-temperature concept to nickel-base and other chromium-bearing alloys, which typically require higher test temperatures and, in some procedures, longer exposure times to initiate attack. Many high-alloy materials show no pitting up to the maximum practicable temperature of the ferric chloride solution, and this is reported accordingly.

Post-Test Evaluation and Reporting

After exposure, specimens are photographed, cleaned per ASTM G1, dried, and reweighed. Pit depths are measured by optical microscopy (using focal-depth difference) or by metallographic cross-sectioning of selected pits. The final report documents alloy grade and product form, heat or lot number, specimen orientation and surface preparation, test method, temperature, duration, mass loss, corrosion rate, pit characterization, and the CPT or CCT where applicable, together with pass/fail conclusions against the specified criteria.

Applications

ASTM G48 testing supports material selection and qualification across industries where chloride-induced localized corrosion is a primary design risk:

  • Oil and gas: qualification of duplex and super duplex tubing, piping, valves, flanges, and subsea components for seawater and produced-fluid service; offshore material specifications such as NORSOK M-630 and qualification frameworks like NORSOK M-650 reference ferric chloride pitting requirements.
  • Desalination and seawater systems: acceptance testing of heat exchanger tubing, condenser components, pumps, and fasteners exposed to chlorinated seawater.
  • Chemical and petrochemical processing: ranking of stainless and nickel-bearing alloys for reactors, columns, and heat exchangers handling chlorides, hypochlorites, and other oxidizing species.
  • Pulp and paper: evaluation of austenitic and duplex grades for bleach plant washers and filters in hot chloride-containing liquors.
  • Power generation and flue gas desulfurization: screening of high-alloy cladding and solid alloys exposed to acidic chloride condensates.
  • Quality control and failure analysis: incoming material verification at accredited third-party laboratories, weld procedure qualification, and comparative assessment of corroded components after service failures.

FAQ

What is the difference between ASTM G48 Method A and Method C?

Method A is a screening test performed at a single fixed temperature for 72 hours, reporting mass loss and whether pitting occurred. Method C is a stepped-temperature procedure that determines the critical pitting temperature, the lowest temperature at which pitting initiates, providing a more quantitative ranking of alloy performance.

What solution is used for ASTM G48 testing?

A ferric chloride solution of approximately 6 % FeCl₃, prepared by dissolving 100 g of FeCl₃·6H₂O in 900 mL of distilled or deionized water. Fresh solution is used for each specimen and for each temperature step in CPT and CCT determinations.

What acceptance criteria are typically specified?

Criteria are set by the purchaser or the governing material specification. Common examples include no visible pitting at a defined magnification, a maximum corrosion rate in mdd, no crevice attack, or a minimum CPT value, such as approximately 40 °C for super duplex and 6 Mo grades in several offshore piping specifications.

How long does ASTM G48 testing take?

Methods A and B require 72 hours of exposure plus specimen preparation, cleaning, and evaluation, typically about one week in total. CPT and CCT determinations involve multiple 24-hour exposures at increasing temperatures and may take from several days up to two weeks depending on the alloy.

Can ASTM G48 results predict service life in seawater?

No. The ferric chloride solution is intentionally much more aggressive than natural seawater, so the test is used for ranking, quality control, and acceptance rather than lifetime prediction. Service assessments should be supplemented with electrochemical tests such as ASTM G61 and ISO 17864, crevice testing per ASTM G78, and engineering judgment.

Is ASTM G48 suitable for carbon steel, aluminum, or coated products?

No. The scope of ASTM G48 is limited to stainless steels, duplex stainless steels, and related nickel- and chromium-bearing alloys that rely on a passive film. Testing of coated parts, carbon steels, or aluminum alloys requires different standards and procedures.

Why Choose ZKGX?

  • State-of-the-art analytical equipment
  • Highly qualified scientific team
  • Fast turnaround time
  • Competitive pricing